宋磊, 王敏, 李新, 高振波, 李小虎, 包燕平. 含锰钢RH真空过程锰的迁移行为[J]. 工程科学学报, 2020, 42(3): 331-339. DOI: 10.13374/j.issn2095-9389.2019.04.08.006
引用本文: 宋磊, 王敏, 李新, 高振波, 李小虎, 包燕平. 含锰钢RH真空过程锰的迁移行为[J]. 工程科学学报, 2020, 42(3): 331-339. DOI: 10.13374/j.issn2095-9389.2019.04.08.006
SONG Lei, WANG Min, LI Xin, GAO Zhen-bo, LI Xiao-hu, BAO Yan-ping. Manganese migration behavior in the RH vacuum process of manganese-containing steel[J]. Chinese Journal of Engineering, 2020, 42(3): 331-339. DOI: 10.13374/j.issn2095-9389.2019.04.08.006
Citation: SONG Lei, WANG Min, LI Xin, GAO Zhen-bo, LI Xiao-hu, BAO Yan-ping. Manganese migration behavior in the RH vacuum process of manganese-containing steel[J]. Chinese Journal of Engineering, 2020, 42(3): 331-339. DOI: 10.13374/j.issn2095-9389.2019.04.08.006

含锰钢RH真空过程锰的迁移行为

Manganese migration behavior in the RH vacuum process of manganese-containing steel

  • 摘要: Ruhrstahl Heraeus(RH)精炼炉是重要的二次精炼装备,但在真空处理过程中会遇到钢液易挥发合金元素的损失量大的问题,且造成钢液真空喷溅的结瘤及对后续钢液的二次氧化。针对含锰钢RH真空处理过程锰的气化导致的元素损失及真空喷溅等问题,跟踪和研究了120 t RH不同真空处理模式下钢液中Mn元素的变化规律及迁移行为。分析了锰元素损失与其挥发和真空喷溅的关系,并在RH真空室内壁不同位置结瘤物的解剖实验中得到验证。研究表明,钢液中Mn元素在RH真空过程中存在着明显损失,真空前期损失量最大;RH真空室内壁结瘤物中锰氧化物的质量分数整体占比高达14%~70%;热力学计算结果显示:温度、钢中Mn的含量以及真空度对Mn的挥发行为均有着很大的影响,是真空过程锰迁移的关键影响因素。通过改进真空压降模式,采用步进式抽真空,元素锰的损失由原先的2×10−4降低至1×10−4,结果对现场生产具有很强的指导意义,通过改进真空压降模式可以有效的抑制钢液的喷溅和挥发,进而减少合金元素锰的损失。

     

    Abstract: The Ruhrstahl Heraeus (RH) refining furnace is a piece of important secondary refining equipment that is widely used in the production of special steel owing to its high efficiency of degassing, decarburization, and de-intercalation. However, molten steel that has a high alloy content will encounter key problems in the vacuum treatment process, and the loss of volatile alloying elements in the molten steel is considerable, resulting in the nodulation of the molten steel vacuum splashing and secondary oxidation of the subsequent molten steel. To address the problems of elemental loss and vacuum splashing caused by manganese (Mn) gasification during the vacuum processing of manganese-containing steel using RH, the variation and migration behavior of Mn in molten steel under different vacuum treatment conditions of 120 t RH were examined. This study analyzed the relationship between manganese elemental loss and its volatilization and vacuum splattering, and it was verified in an anatomical experiment of the nodule at different positions inside the RH vacuum chamber. The results show that elemental Mn in the molten steel shows obvious loss during the vacuum process of RH, and the loss in the early stage of the vacuum process is the largest. The composition of manganese oxide in the nodule of the RH vacuum chamber is as high as 14%–70%, and the thermodynamic calculation results show that temperature, the content of Mn in the steel, and the degree of vacuum have a considerable influence on the volatilization behavior of Mn, which is the key influencing factor for manganese migration during the vacuum process. By improving the vacuum pressure drop mode, a stepwise vacuum is used to reduce the loss of elemental Mn from the original 2×10−4 to 1×10−4. The results have considerable significance for on-site production, and steel can be effectively restrained by improving the vacuum pressure drop mode. Additionally, the splashing and volatilization of liquid reduces the loss of the alloying element Mn.

     

/

返回文章
返回