Synthesis and characterization of kalsilite powder using a fast sol-gel method
-
-
Abstract
Nitrate replaced alkoxide and alcohol solvent omitted, a TEOS-KNO3-Al(NO3)3-H2O system turned into gel in 5~12 min with pH adjusted by aqua ammonia. Dried gel treated at 862℃, pure and homogeneous kalsilite powder was prepared with an average particle size of 8μm. The TEOS hydrolysis reaction was catalyzed by H+ released from aluminum nitrate hydrolysis firstly, and then promoted again by OH- with the addition of aqua ammonia. The gelation time was shortened greatly owing to the catalysis mode of acid first and alkali second. A penta-coordination Al was detected by 27Al NMR analyzing the dried aluminosilicate gel.
-
-